Stainless Steel 347 1.4550
Haec notitia schedae applicatur ad ferrum incorruptum 347 / 1.4550 linteum calidum et frigidum involutum, habena et vectes, producta semi-perfecta, virgas et sectiones necnon inustibilem et conflati fistulae ferreae ad machinationem mechanicam et generalem proposita.
Applicationem
Partes enim constructiones, quae scalis usque ad 1050°C resistere debent et effectui gasorum sulphureorum late insuetae, praesertim supra 900°C, valde infimae sunt.
Chemical Compositions*
Elementum | % Praesens (in product form) |
---|---|
Carbon (C) | 0.08 |
Pii (Si) | 1.00 |
Manganum (Mn) | 2.00 |
Phosphorus (P) | 0.041 |
Sulphur (S) | 0.014 |
Chromium (Cr) | 17.00 – 19.00 |
Nickel (Ni) | 9.00 – 12.00 |
Niobium (Nb) | 10xC ad 1.00 |
Ferrum (Fe) | Libra |
Mechanica proprietatibus (ad locus temperatus in annealed conditione)
Product Form | ||||||||
---|---|---|---|---|---|---|---|---|
C | H | P | L | L | TW / TS | |||
Crassitudo (mm) Max | 8 | 13.5 | 75 | 160 | 2502) | 60 | ||
Cedat imperium | Rp0.2 N/mm2 | 2203) | 2003) | 2003) | 2054 | 2056) | 2055) | |
Rp1.0 N/mm2 | 2503) | 2403) | 2403) | 2404) | 2406) | 2405) | ||
Distrahentes fortitudo | Rm N/mm2 | 520 – 7203) | 520 – 7203) | 500 – 7003 | 510 – 7404) | 510 – 7406 | 510 – 7405) | |
Prolongatio min.in & | A1)% min (longitudinalis) | - | - | - | 40 | - | 35 | |
A1)% min (transversus) | 40 | 40 | 40 | - | 30 | 30 | ||
Impact Energy (ISO-V) ≥ 10mm crassum | Jmin (longitudinalis) | - | 100 | 100 | 100 | - | 100 | |
Jmin (transversus) | - | 60 | 60 | - | 60 | 60 |
Reference data in aliqua physica
Densitas in 20°C kg/m3 | 7.9 | |
---|---|---|
Modulus Elasticitatis kN/mm2 at | 20°C | 200 |
CC°C | 186 | |
400°C | 172 | |
500°C | 165 | |
Scelerisque Conductivity W/m K ad 20°C | 15 | |
Imprimis Scelerisque capacitas ad 20°CJ/kg K | 500 | |
Resistivity Electrical in 20°C Ω mm2 /m | 0.73 |
Coefficiens linearum scelerisque expansionem 10-6 K-1 inter XX ° F et
100°C | 16.0 |
---|---|
CC°C | 16.5 |
300°C | 17.0 |
400°C | 17.5 |
500°C | 18.0 |